Chemical Composition of Deposited metal (%):
| C | Mn | Si | P | S | Ni | Mo | |||
| Range | ≤0.12 | ≤1.75 | ≤0.8 | ≤0.030 | ≤0.030 | 0.80~1.20 | ≤0.35 | ||
| Test | 0.04 | 1.40 | 0.38 | 0.013 | 0.009 | 0.90 | 0.001 |
Mechanical properties of deposited metal:
| Tensile strength Rm (Mpa) | Yield strength Rp0.2 (Mpa) | Elongation ratio (%) | AKV(-30℃) | Shielding gas | |||||||
| Range | 550-740 | ≥460 | ≥17 | ≥27 | 100%CO2 (purity≥99.8%) | ||||||
| Test | 620 | 565 | 25 | 100 | |||||||
Diffusion hydrogen content of deposited metal (Measured value): 5.6ml/100g
Reference Current (DC+)
| Diameter of welding wire (mm) | φ1.2 | φ1.4 | φ1.6 | ||||||||
| Current range (A) | Flat welding | 120~300 | 150~400 | 180~450 | |||||||
| Upward vertical welding, overhead position welding | 120~260 | 150~270 | 180~280 | ||||||||
| Vertical down welding | 200~300 | 220~300 | 250~300 | ||||||||
| Horizontal position welding | 120~280 | 150~320 | 180~350 | ||||||||
Precautions:
- The work piece shall be degreased and derusted before welding.
- When welding, the gas flow rate is generally 20~25L/min
- the dry extension lengh of the wire should be 15~25mm while the wire welding.